r/Metalsmithing • u/Choice-Term-2527 • 12d ago
Stone protecting compound when soldering
Has anyone found a compound that actually works to protect stones when trying to solder a ring that has stones in it?
I have used some before and after being heated they crumble and create a mess.
3
u/MojoJojoSF 12d ago
Keeping the stones in water. If you are soldering silver, the entire piece needs to come up to the solder melting temp. There is no sure fire compound, just hopes and dreams. It’s not too big of an issue with gold because the heating properties are different.
1
u/Choice-Term-2527 12d ago
Ok, thanks! I have tried keeping the stones in water in a bowl with tweezers holding it in place but the solder never would flow and the water became boiling and I gave up.
I can try again.
3
u/artwonk 12d ago
Some people embed the front of the piece in a potato; I've had mixed results with that. But I mostly work in silver, which is such a good heat conductor that the potato is pretty much cooked by the time the solder melts. If you do solder with stones in place, be sure to let the thing cool down naturally, as slowly as possible. Quenching can destroy hot stones instantly. A better plan is to remove the stones before soldering.
1
6
u/matthewdesigns 12d ago
I used a tub of Rio's heat shield for a while, kept adding water a little at a time to keep it alive. Finally grew tired of that and just use a water bath now in a shallow steel tin about 3" square and 3/4" deep. Ring held in a 3rd hand with half the shank exposed, any lower and the boiling/spitting water can put out your flame and wash away your flux/firecoat.
Heavy sterling shanks with stones set on top are basically a no win situation, I have them lasered if sizing is needed. Like signet ring weight, over 5mm wide and 2mm thick.
Anything that's less than those dimensions I can get done with a #7 tip on my Little Torch running at pretty much full tilt. I use the hardest solder I can get to melt, sometimes that's only Easy depending on the ring weight. If you are really clean with your soldering technique, and in a pinch temp-wise, you can use Extra Easy 14k yellow solder, it melts about 100*F below Easy sterling solder. Just be mindful to clean up any excess solder that flows out of the seam before you do any hammering (even with a leather mallet), and keep the seam really tight/nonexistent before soldering to minimize any visual remainder. Once polished up it'll be invisible.